What defects will be formed when the pouring temperature of gray cast iron is too low?

Time:2021-11-25 10:14:03 Author:Daguang JinpengClick:56

In the casting process of gray cast iron,the molten iron temperature can be well controlled by induction furnace melting.If the pouring temperature is too high,the sand mold will expand,especially the gray cast iron castings with complex sand core.When the pouring temperature is≥1420℃,the scrap increases,and when the pouring temperature is 1460℃,the scrap reaches 50%.So what defects may be formed when the temperature is too low,and what are the causes and solutions of the defects?

(1)Manganese sulfide porosity.

Cause of defect:this kind of air hole is located below the gray cast iron casting.The cast iron processing plant is mostly on the casting surface,which is often exposed after processing,with a diameter of about 2~6mm.Sometimes there is a small amount of slag in the tunnel.Metallographic study shows that this defect is caused by MNS segregation and slag mixing,which is caused by low pouring temperature and high content of manganese and sulfur in molten iron.

Solution:such s content and appropriate Mn content(0.5%~0.65%)can

The purity of molten iron is significantly improved,so that the effect is excellent and such defects are prevented.

(2)Porosity caused by sand core gas.

Defect cause:pores and porous pores are often caused by poor exhaust of sand core.Because the sand core is hardened in the core box when the iron casting factory makes the core,the exhaust hole on the sand core is often insufficient.

Solution:in order to form an exhaust hole,additional drilling can be done after the core is hardened.

(3)Liquid slag inclusion.

Defect cause:it is worth mentioning that changing the gating system design failed to eliminate this defect.Therefore,this defect can be considered as the result of low pouring temperature and molten iron pouring in micro reducing atmosphere.After processing,there will be individual small holes under the skin of gray cast iron castings,and the diameter of the holes is generally 1~3mm.In some cases,there are only 1~2 small holes.Metallographic study shows that these pores appear together with a small amount of liquid slag,but no s segregation is found here.

Solution:the research shows that this defect is related to the pouring temperature.When the pouring temperature is higher than 1380℃,this defect is not found in the casting,so the pouring temperature should be controlled at 1380~1420℃.

Conclusion:the common reason for the low pouring temperature is that the molten iron is transported and stays in the open ladle for a long time to dissipate heat before pouring.The use of ladle covers with thermal insulation can significantly reduce heat loss.

prev:none